ISO 5636 Explained: Air Permeance Test Methods for Paper

An air permeability tester for paper should be selected against the test method and the material’s expected air flow—not just the instrument’s advertised range. Two testers can measure the same sheet and produce different-looking results because they apply different pressures, measure different quantities, or seal the specimen differently. For technical evaluators, the first decision is therefore which ISO 5636 method the result needs to satisfy.

ISO 5636 covers methods for determining the air permeance of paper and board under specified conditions. The Bendtsen and Gurley methods are widely recognized approaches within the series, but their results are not interchangeable by a simple universal conversion. Understanding that distinction helps laboratories choose equipment that supports meaningful quality control, supplier comparisons, and material specifications.

Air permeance and air resistance: what the result represents

Air permeance describes how readily air passes through a material under a pressure difference. In principle, a more permeable sheet allows more air through for a given test area, pressure difference, and time. Air resistance describes the opposing behavior: a sheet that slows air passage produces greater resistance.

In paper testing, however, the reported number depends on the method. A flow-based instrument may report the volume of air passing through a specimen over time under specified conditions. A Gurley-type instrument commonly reports the time required for a specified volume of air to pass through the test area. A longer Gurley time indicates greater resistance under that method’s conditions.

A time result in seconds is not the same quantity as air permeance. Converting or comparing results requires attention to the method’s pressure conditions, test area, flow behavior, and reporting conventions. Treating a Gurley time and a Bendtsen flow reading as equivalent can lead to incorrect material acceptance decisions.

ISO 5636 test methods: Bendtsen and Gurley compared

The following comparison focuses on how the methods generate a result and what that means for equipment selection.

ConsiderationISO 5636-3: Bendtsen methodISO 5636-5: Gurley method
Measurement approachMeasures air flow through the test piece under a specified pressure difference.Measures the time required for a specified volume of air to pass through the test piece under the instrument’s pressure conditions.
Typical reported resultAir flow rate, expressed according to the method and instrument.Air passage time, commonly called Gurley time or Gurley air resistance.
Direction of changeGreater flow generally indicates a more air-permeable sheet.Longer passage time indicates greater air resistance.
Equipment evaluation focusFlow range, pressure control, sealing, and resolution at the expected flow.Measurable passage-time range, timing, pressure conditions, and sealing.

Bendtsen: evaluating flow through the sheet

The Bendtsen method is useful when a laboratory needs a flow-based assessment of paper or board. The instrument applies a specified pressure difference across a clamped test piece and measures the resulting air flow. The method is sensitive to both the sheet’s structure and the integrity of the seal around the test area.

For equipment selection, the important question is whether the expected flow falls comfortably within the instrument’s usable range. If the paper allows very little air through, a flow reading near the lower limit may be difficult to distinguish from leakage or measurement noise. At the other extreme, a very open sheet can exceed the instrument’s practical flow range. In either case, a nominal claim of method support does not establish suitability for every paper grade.

Gurley: evaluating the time taken for air to pass

The Gurley method expresses the result as the time taken for a specified volume of air to pass through the specimen. This makes it useful where a material specification or established quality-control record is written in Gurley time.

The usable test-time range matters. A highly open paper may allow the specified volume to pass so quickly that timing and specimen handling have a disproportionate effect on the result. A very resistant sheet may require a long test or fall outside the instrument’s practical capability. Evaluators should consider both extremes if the laboratory handles several grades.

A Gurley result also reflects the pressure conditions of the method. It should not be treated as if it were measured under the same conditions as a constant-pressure flow test merely because both tests concern air passing through paper.

How to select an air permeability tester for paper

Begin with the result that must be reported. If a customer specification, purchase agreement, or internal control plan calls for a particular ISO 5636 part, the equipment must support that method and its required test conditions. An instrument that measures a similar property by a different principle may be useful for development, but it cannot automatically replace the specified test.

Next, compare the instrument’s working range with representative materials, including the most open and most resistant grades. Ask for the range in the same quantity used for the acceptance decision: flow for a flow-based method, or passage time for a time-based method. Resolution should also be adequate to distinguish meaningful changes around the specification limit, rather than merely display additional digits.

The specimen clamp deserves as much attention as the measuring system. Rough, embossed, stiff, or uneven materials can be difficult to seal consistently. Air escaping around the test area may be interpreted as flow through the sheet, making the material appear more permeable than it is. A secure seal should not require crushing or damaging the sheet in a way that changes its structure.

For laboratories comparing suppliers or production sites, continuity with existing records is another selection criterion. Changing the method, test area, or reporting quantity can shift the apparent baseline even when the material has not changed. Before replacing an established method, test representative samples with both arrangements and evaluate the relationship across the relevant material range. That comparison can support an internal transition, but it does not create a universal conversion between methods.

Paratronix Instruments Co., Ltd. provides packaging testing instruments and testing solutions for a range of materials. When discussing a paper-testing application with an equipment supplier, provide the required ISO method, paper grades, expected result range, and reporting needs so the proposed configuration can be assessed against the actual test.

Specimen condition can change the result

Paper is sensitive to moisture and handling. Changes in ambient conditions can alter sheet dimensions and structure, affecting the passage of air. Specimens should therefore be conditioned and tested under the conditions required by the applicable method and associated conditioning requirements. When comparing results from different laboratories, the conditioning history is part of the comparison, not an administrative detail.

Sampling also affects the usefulness of a reported value. A single spot may not represent a sheet with local variation, visible defects, or differences across its width. Follow the applicable sampling and test requirements, and preserve the individual readings when investigating variation. An average can conceal isolated weak areas or inconsistent sealing.

Handle specimens so that folds, punctures, contamination, and compressed areas do not influence the test area unless those features are deliberately part of the investigation. For coated or layered materials, record the specimen orientation and test arrangement. A repeatable setup is essential when comparing results over time, even where both sides appear visually similar.

When results disagree: a practical investigation

A disagreement between two air-permeance results does not immediately establish that one instrument is faulty. Start by checking whether the laboratories used the same method and reported the same quantity. A flow result and a passage-time result answer related questions, but their numerical values cannot be compared directly.

If the method is the same, examine specimen selection and condition. Different locations on a roll or sheet, different conditioning histories, and damaged test areas can all produce variation. Compare individual measurements rather than only the reported averages; a wide spread may point toward material nonuniformity or an inconsistent seal.

Then assess the measuring arrangement. Check the clamp and contact surfaces for contamination or wear, review the instrument’s calibration and maintenance records, and investigate whether the expected result is close to a range limit. A leak can have a particularly large effect when the true flow through the material is low. Conversely, a very short timed test can make small differences in timing more influential.

If both systems appear sound, test a common set of representative specimens using an agreed sampling and conditioning procedure. A consistent difference across grades may indicate a systematic difference in setup or measurement. A difference that appears only for rough or stiff sheets points more strongly toward specimen contact or sealing.

What air permeance does—and does not—establish

Air permeance is a useful indicator of how air moves through the tested material under a defined set of conditions. It can support process control, grade comparisons, and investigation of changes in paper structure when the same method and specimen preparation are used consistently.

It does not by itself establish a packaging material’s barrier performance against water vapor, individual gases, liquids, or microorganisms. Those properties involve different transport mechanisms, test conditions, or both. A paper that resists air passage in an ISO 5636 test should not automatically be assigned a particular performance level for another barrier requirement.

For a technical evaluation, the strongest equipment choice is the one that measures the specified quantity reliably across the materials the laboratory actually tests. Define the required ISO 5636 method, verify that representative specimens fall within the instrument’s working range, and assess sealing and repeatability before using results to set or enforce material limits.

NEXT:Already the last page